SUS431 ● Chemical Composition: Carbon C: 0.11 ~ 0.17 Si Si: ≤0.80 Manganese Mn: ≤0.80 Sulfur S: ≤0.030 Phosphorus P: ≤0.035 Chromium Cr: 16.00 ~ 18.00 Ni Ni: 1.50 ~ 2.50 ● Mechanical Properties: Tensile strength σb (MPa): quenching and tempering, ≥1080 Elongation δ5 (%): quenching and tempering, ≥10 Impact energy Akv (J): quenching and tempering, ≥39 Hardness: annealing, ≤285HB
● range SUS431 characteristics and application: as having a higher resistance to nitric acid and organic acid corrosion of parts, containers and equipment.
● Heat treatment and microstructure specifications: Heat treatment specifications: 1) annealing, 680 ~ 700 ℃ tempering air-cooled; 2) quenching, 950 ~ 1050 ℃ oil cooling; 3) 275 ~ 350 ℃ tempering air cooling. Microstructure: Organizing for the martensite type. ● Delivery status: to heat treatment delivery in general, the treatment types specified in the contract; not indicated, by not heat treatment delivery.
|