Stainless steel: SUS321
● Features and Scope: Add Ti improve resistance to intergranular corrosion, is not recommended for decorative parts. ● Chemical Composition: Carbon C: ≤0.08 Si Si: ≤1.00 Manganese Mn: ≤2.00 Sulfur S: ≤0.030 Phosphorus P: ≤0.035 Chromium Cr: 17.00 ~ 19.00 Ni Ni: 9.00 ~ 12.00 Titanium Ti: ≥5 × C% ● Mechanical Properties: Tensile strength σb (MPa): ≥520 Conditions yield strength σ0.2 (MPa): ≥205 Elongation δ5 (%): ≥40 Reduction of ψ (%): ≥50 Hardness: ≤187HB; ≤90HRB; ≤200HV ● Heat treatment and microstructure specifications: Heat treatment specifications: 1) solid solution 920 ~ 1150 ℃ rapid cooling; 2) According to the requirements may be stabilizing treatment, heat treatment temperature is 850 ~ 930 ℃, but it must be stated in the contract. Microstructure: Organizing for the austenitic type. ● Delivery status: to heat treatment delivery in general, the treatment types specified in the contract; not indicated, by not heat treatment delivery. |
|
|
|
|
|
|
|
|