Quality carbon structural steel: C40 (1.0511) Implementation of the standards: EN 10083 / 2-1991 ● Features and Scope: Welding performance is poor, for the manufacture of wear parts such as shafts and gears. ● Chemical Composition: Carbon C: 0.37 ~ 0.45 Si Si: 0.17 ~ 0.37 Mn Mn: 0.70 ~ 1.00 Sulfur S: ≤0.045 Phosphorus P: ≤0.045 Chromium Cr: ≤0.40 Ni Ni: ≤0.40 Mo Mo: ≤0.10 ● Mechanical Properties: Tensile strength σb (MPa): ≥590 (60) Yield strength σs (MPa): ≥355 (36) Elongation δ5 (%): ≥17 Reduction of ψ (%): ≥45 Impact energy Akv (J): ≥47 Impact toughness αkv (J / cm2): ≥59 (6) Hardness: no heat, ≤229HB; annealed steel, ≤207HB Sample size: Sample size is 25mm ● Heat treatment and microstructure specifications: Heat treatment specifications: normalizing, 860 ℃; quenching, 840 ℃; tempering, 600 ℃. ● Delivery status: to heat or no heat treatment (annealing, normalizing or tempering) state delivery. Require heat treatment delivery should be specified in the contract, no heat treatment is not indicated by delivery. |
|
|
|
|
|
|
|
|